Home > Products & Services > Plastics > Technical publications

Processing guide : Staple Fibre Compact Process



Settings
Melt Temperature 240º - 280ºC
Dowtherm / Diphyl Temp. 230º - 275ºC
Cooling Air 15º - 20ºC
Slow Godets Temp. 80º - 120ºC
Fast Godets Temp. 40º - 60ºC
Draw Ratio 1: 3.0 – 4.5
Line Speed Up to 160 m/min
Our Grades for Spinning Staple Fibres
SABIC® PP 510A – MFR 10.5 g/10 min – Anti Gas Fading
– For Coarse Fibres > 2.8 dtex
SABIC® PP 513A – MFR 6.0 g/10 min – Anti Gas Fading
– For High Tenacity Fibres: 3.3 to 6.7 dtex
SABIC® PP 515A – MFR 24 g/10 min – Anti Gas Fading
– For Micro Fibres: 0.6 to 2.8 dtex

Other processing guides :

Select here
Select here